Fri, 16 October, 2026
Welding Automation in Shipbuilding
By David W Millar CEng MPhil CEWE CIWE FWeldI
The need to remain competitive in the international shipbuilding market has encouraged the development of new fabrication techniques, welding processes and working practices. With increasing demand for naval and commercial vessels, shipyards are seeking ways to improve productivity while maintaining the high standards of weld quality required for large, complex marine structures.
Welding automation has become an important part of this development. From relatively simple mechanised welding tractors to sophisticated robotic systems, automation offers opportunities to reduce production time, improve consistency and make more effective use of skilled personnel.
However, the benefits of automation depend on more than the welding equipment itself. Successful implementation requires appropriate joint preparation, operator training, production planning and an understanding of the relationship between welding technology and the wider shipbuilding process.
The Need for Greater Welding Productivity
Shipbuilding has experienced increasing demand for vessel tonnage, including substantial naval construction programmes in countries such as Canada, the United States, the United Kingdom, Australia and India.
This growth has placed pressure on shipyards to increase output while controlling fabrication costs.
Welding represents a significant proportion of the work involved in constructing a ship. Large hull structures contain extensive butt and fillet welds, while internal stiffeners, webs, girders and bulkheads introduce numerous additional joints.
Consequently, improvements in welding productivity can have a considerable influence on overall construction efficiency.
A further challenge is the availability of skilled labour. Many shipyards have experienced difficulties recruiting sufficient qualified welders to meet production requirements.
These pressures have encouraged the adoption of welding processes that can be mechanised or automated more readily than traditional manual techniques.
The importance of collaboration between shipbuilders and equipment manufacturers was recognised in Japan during the 1980s, when working groups were established involving shipyard welding departments, welding equipment manufacturers and consumable suppliers.
Their objective was to develop welding processes and automation systems that could improve productivity while addressing limitations in skilled labour availability.
Welding Processes and Operator Training
The transition from manual to mechanised welding often begins with the selection of processes suitable for continuous wire feeding.
Shielded Metal Arc Welding (SMAW) has traditionally been widely used in fabrication because of its relatively simple equipment requirements and operational flexibility.
A typical SMAW installation consists of a power source, welding cables and an electrode holder. Equipment adjustment is comparatively straightforward, and the process can be used in a variety of working environments.
However, the process requires frequent electrode replacement and relies heavily on the manual skill of the welder.
Gas-shielded flux cored arc welding (FCAW) and metal cored arc welding offer opportunities for increased productivity through continuous wire feeding.
These processes are also well suited to mechanisation.
The equipment is generally more complex than a conventional SMAW installation. Parameters such as welding current, voltage, wire feed speed and shielding gas conditions must be controlled appropriately.
Incorrect settings can adversely affect weld quality, making effective operator training essential.
Although semi-automatic welding can increase deposition rates and reduce interruptions, greater productivity gains become possible when the welding torch is supported and moved by a mechanised system rather than being manipulated entirely by the welder.
This allows the operator to concentrate on monitoring the welding operation and managing equipment rather than continuously controlling torch movement.
The Importance of Joint Preparation
One of the fundamental requirements for successful welding automation is consistent joint preparation.
Manual welders can make adjustments to accommodate variations in fit-up and joint geometry. Mechanised welding equipment generally has less flexibility unless additional sensing and adaptive control systems are provided.
Consequently, inconsistent preparations can lead to variations in weld quality and reduce the benefits of automation.
Shipyards can improve preparation quality through controlled cutting and edge preparation.
Oxy-fuel and plasma cutting systems can produce repeatable joint geometries when correctly set up and maintained.
Portable bevelling machines provide another solution, particularly for large plates and structures where movement to a fixed preparation station may be impractical.
These machines can produce accurate weld preparations without introducing the heat associated with thermal cutting. Their portability also allows preparation work to be carried out at different locations within the fabrication area.
An operator may be able to supervise several machines simultaneously, improving the utilisation of available labour.
Consistent preparation is therefore not simply a quality requirement; it is an important contributor to welding productivity.
Mechanised Fillet Welding
One of the simplest approaches to welding automation involves mounting a welding torch on a lightweight, self-propelled tractor.
These systems are particularly suitable for repetitive fillet welds, which are common throughout ship structures.
A mechanised tractor can maintain a relatively consistent travel speed and torch position, helping to produce repeatable weld profiles.
Welding consumables may be supplied through portable wire feeders or larger wire delivery systems.
The use of large wire drums, including 200 kg supply packs, can reduce interruptions associated with consumable replacement.
In suitable applications, one operator may be able to supervise two or more welding tractors.
Double-headed arrangements can also permit fillet welding on both sides of a joint.
Such systems illustrate that automation does not necessarily require a large capital investment or a sophisticated industrial robot.
Relatively straightforward equipment can provide worthwhile improvements when applied to appropriate repetitive welding operations.
Improving Productivity with Welding Oscillators
Welding in the flat position is generally preferred because it offers favourable conditions for productivity and weld pool control.
Shipbuilding production planning therefore seeks to maximise the amount of welding that can be completed in this position.
Nevertheless, the geometry and assembly sequence of large hull structures mean that welding must also be carried out in horizontal, vertical and overhead positions.
Mechanised oscillation systems can provide advantages in these more demanding applications.
A welding oscillator moves the torch across the joint according to a controlled pattern while the carriage travels along the weld.
This arrangement can help maintain consistent bead placement and provide a repeatable technique for filling the joint.
A Shipyard Application in Glasgow
An example described in the original article concerns the welding of large hull block connections at a shipyard in Glasgow.
The yard assembled major hull sections containing numerous webs, girders and longitudinal members.
Traditionally, the bottom shell connection was welded from inside the vessel using a single-V joint preparation and ceramic backing.
Although this approach avoided the need for back gouging, it presented several practical difficulties.
Access for welders was restricted by internal structural members, and welding through openings in webs and girders could be particularly challenging.
The alternative approach involved reversing the joint preparation and carrying out the principal welding operation from outside the hull.
A root pass was deposited from inside against ceramic backing, after which a mechanised welding tractor and oscillator were used to complete the joint externally with flux cored welding wire.
This required overhead welding on the bottom shell, with the welding position changing as the joint continued towards the side shell.
A flexible track enabled the welding carriage to follow the changing geometry.
The results demonstrated the potential benefits of combining mechanisation with a revised fabrication method.
When compared with the previous procedure, planned welding man-hours were reduced by 72%.
The completed welds also exhibited high visual quality, while radiographic examination results were consistently improved.
These benefits depended on two particularly important elements: a reliable oscillation system and high-quality all-positional flux cored welding consumables.
The example demonstrates that the most effective use of automation may involve changing the location and sequence of welding operations rather than simply replacing manual torch movement.
Applications Beyond Hull Butt Welds
Mechanised welding oscillators can be adapted to a range of joint configurations.
Systems are available for welding in horizontal and other positions, including applications involving ceramic backing.
Track-mounted carriages can also support operations other than welding.
For example, oxy-fuel or plasma cutting torches may be mounted on a carriage to perform controlled cutting or preparation operations.
Inspection equipment can also be positioned using a track system.
In pipe fabrication, a fixed track may be attached around the circumference of a pipe, allowing one or more mechanised welding heads to travel around the joint.
This flexibility allows shipyards to use related mechanisation technologies across different fabrication and maintenance tasks.
Panel Line Systems and Robotic Welding
Panel lines represent another major opportunity for automation in shipbuilding.
Large flat panels form the basis of many hull structures. They are subsequently fitted with stiffeners and other reinforcing members before being incorporated into larger blocks.
Because panel fabrication contains repetitive operations, it is particularly suitable for mechanised and robotic welding.
However, increasing the welding speed does not automatically improve the productivity of the entire panel line.
If upstream operations, such as fitting and positioning stiffeners, cannot keep pace with welding, a production bottleneck may develop.
Simulation tools can help identify these constraints and evaluate changes to the manufacturing sequence.
In some circumstances, the optimum short-term solution may even involve reducing welding speed until the surrounding production operations can be improved.
This highlights the importance of considering the complete fabrication process when introducing automation.
Developments in Robotic Programming
Industrial robots have been used in shipbuilding for many years, but their application has historically been limited by programming requirements.
Traditional robotic welding systems often rely on computer-aided design information or manually taught welding paths.
In a teaching operation, the welding head is moved through the required positions and the resulting information is stored for future use.
Although effective for repeated production of identical components, this approach can become time-consuming when joint geometry or component positioning changes frequently.
Shipbuilding presents particular difficulties because large fabricated structures may exhibit dimensional variation, and production often involves relatively low volumes of highly complex assemblies.
Modern sensing and control technologies are helping to address these limitations.
Vision-Based Robotic Welding
The original article describes the Inrotech-Micro Twin system as an example of simplified robotic operation.
Rather than requiring extensive manual programming for every component arrangement, the system uses scanning and sensing to identify the positions of items within its working area.
Components can be placed within the operating footprint, after which the system scans the assembly and determines the location of the joints to be welded.
The published example reports a typical scanning time of less than five minutes, with scanning speeds of approximately 8 m/min.
A laser sensor verifies the position of the structural members before welding begins.
The equipment incorporates the welding torch and fume extraction arrangement, while the operator uses an intuitive control interface to initiate the process.
The article also describes opportunities for remote operation and remote diagnostics.
For the installation discussed, the anticipated return on investment was approximately one to two years.
These figures relate to the equipment and application described in the original publication and should not be treated as universal performance guarantees.
The wider significance of such systems is their potential to reduce the programming effort associated with robotic welding.
This can make automation more attractive for shipyards dealing with variable component geometries and complex fabrication requirements.
Designing Structures for Robotic Manufacture
The introduction of robotic welding has implications for designers and production planners.
A component that is straightforward to weld manually may not necessarily be well suited to robotic fabrication.
Access restrictions, joint positioning, assembly sequence and the arrangement of structural members can all influence whether a robot can complete the required operation.
To realise the full benefits of robotic welding, shipyards must therefore consider automation during the design and planning stages.
Fabrication drawings and assembly instructions should take account of the intended welding equipment.
This may involve revising joint configurations, adjusting production sequences or ensuring that suitable access is available for robotic welding heads.
The objective is to reduce not only the time required to deposit weld metal but also the total time needed to complete a fabricated assembly.
Automation in Weld Repair and Finishing
Automation also has applications when welding does not proceed as intended.
Even with modern equipment and carefully controlled procedures, weld defects can occur and repairs may be necessary.
Repair preparation often involves removing defective weld metal through gouging, grinding or other material removal processes.
These operations can be labour-intensive and may expose workers to noise, dust and fumes.
Mechanised systems can improve consistency and reduce the manual effort involved.
The original article describes a track-mounted automatic gouging system capable of producing controlled gouge geometry.
Reported performance included gouging speeds up to five times faster than manual methods and a reduction in subsequent grinding of approximately 90%.
These improvements can also reduce the time and consumables required to complete repair work.
Automated weld shaving equipment provides another example.
A track-mounted machine can remove excess weld metal or weld caps at controlled speeds while reducing some of the noise, dust and heat associated with manual finishing.
The equipment described in the article was reported to achieve weld cap removal speeds of up to 37 metres per hour.
Such systems demonstrate that the potential benefits of automation extend beyond weld deposition to preparation, repair and finishing.
Collaborative Robots and the Future of Shipbuilding
A further development is the use of collaborative robots, commonly referred to as cobots.
These systems are intended for applications involving interaction or proximity between people and robotic equipment.
Unlike traditional industrial robots, which are commonly separated from personnel by protective enclosures, collaborative robotic systems can be designed to operate in shared workspaces when appropriate safeguards are provided.
Their suitability depends on the particular application and the associated safety assessment.
For shipbuilding, mobile robotic systems offer particular advantages because workpieces are often too large to be moved conveniently to a fixed robotic station.
A mobile robot can potentially be taken to the structure, rather than requiring the structure to be transported to the robot.
This creates opportunities for welding within large hull sections, compartments and other difficult-to-access areas.
High-Mobility Manufacturing Robots
An example discussed in the original article is the High-Mobility Manufacturing Robot developed by Robotic Technologies of Tennessee.
The system combines a lightweight robotic welding arm with a mobile climbing platform.
It is designed to be transported and deployed for a range of manufacturing tasks, including welding operations in shipbuilding and other heavy engineering sectors.
The robot can operate on flat, vertical and horizontal surfaces and transition between different planes.
Onboard lidar technology supports mapping and obstacle avoidance, while a touch-panel interface enables remote control of welding operations.
The original article reports development and demonstration work supported by the National Shipbuilding Research Program in the United States.
This included fillet welding in the 2F and 3F positions on compartments and stiffeners, with the welding requirements validated and tested by the Edison Welding Institute.
Such developments illustrate the potential for automation to move beyond conventional fixed production lines.
Mobile robotic welding may be particularly valuable where access is restricted or where removing personnel from a hazardous working environment offers safety advantages.
The Importance of an Integrated Approach
The adoption of welding automation is not simply a question of replacing a welder with a machine.
Productivity improvements depend on the interaction between welding processes, consumables, equipment, joint preparation, fabrication planning and operator competence.
A mechanised welding tractor may provide an effective solution for repetitive fillet welds.
An oscillator may allow a major hull connection to be completed more efficiently by changing the welding position and access arrangements.
Vision-based robotic systems can reduce programming requirements, while mobile robots offer possibilities for working directly on large and complex structures.
Each technology addresses a different manufacturing requirement.
The most appropriate choice depends on the nature of the work, the production volume, the degree of dimensional variation and the resources available to the shipyard.
Importantly, the successful introduction of automation does not eliminate the need for welding expertise.
Skilled personnel remain essential for developing welding procedures, selecting suitable consumables, maintaining equipment, evaluating weld quality and managing the overall fabrication process.
Conclusion
As demand for shipbuilding capacity increases, manufacturers must continue to identify methods of improving welding productivity without compromising quality.
Mechanised welding, robotic systems and advanced sensing technologies provide opportunities to address these requirements.
The examples discussed demonstrate that substantial improvements can be achieved through relatively simple automation, particularly when it is combined with changes to joint design and fabrication methods.
More sophisticated robotic systems offer further possibilities, especially where they can accommodate dimensional variation and reduce programming effort.
The continuing development of mobile and collaborative robotics may also allow automation to be applied in areas of ship construction that have traditionally depended on manual welding.
Ultimately, the greatest benefits will be achieved by shipyards that treat welding automation as part of an integrated manufacturing strategy, rather than as an isolated equipment investment.
Originally published in: Welding and Joining Matters, Issue 7, January 2024, pages 13–15.