Welding procedure qualification is a fundamental part of quality assurance in welded fabrication. It provides documented evidence that a proposed welding procedure can produce a joint with the required mechanical properties and acceptable weld quality.
For manufacturers working to European and international standards, BS EN ISO 15614-1 is one of the principal specifications governing the qualification of welding procedures for steels and nickel alloys.
However, the qualification process involves more than producing a satisfactory test weld. It requires an understanding of essential variables, ranges of approval, inspection requirements and the documentation needed to support subsequent production welding.
This article examines the principal requirements of welding procedure qualification to BS EN ISO 15614-1, concentrating on Level 2 qualification and the practical considerations that can influence the cost and usefulness of a procedure test.
Welding Procedure Qualification Standards
Two principal systems are commonly used to qualify welding procedures: the ISO series of standards and the ASME Boiler and Pressure Vessel Code.
The ISO 15614 series provides requirements for welding procedure qualification across different materials and welding processes.
BS EN ISO 15614-1 specifically addresses arc and gas welding of steels and arc welding of nickel and nickel alloys.
The standard is widely used where European or international welding requirements apply.
The edition discussed in the original April 2025 article was BS EN ISO 15614-1:2017+A1:2019.
Level 1 and Level 2 Qualification
ISO 15614-1 specifies two levels of welding procedure qualification.
Level 1 is based on the approach used in ASME Section IX, while Level 2 follows the requirements established in earlier editions of ISO 15614-1.
Qualification to Level 2 also provides qualification to Level 1, but the reverse does not apply.
Where neither the contract nor the application standard identifies a particular level, Level 2 is the default.
The original article also notes the relevance of Level 2 qualification to conformity with applicable pressure equipment requirements.
Manufacturers must therefore establish which qualification level is required before beginning testing.
The remainder of this article concentrates on Level 2.
The Procedure Qualification Process
A typical welding procedure qualification involves several stages, beginning with preparation of a preliminary welding procedure specification and ending with the issue of a welding procedure qualification record.
The preliminary welding procedure specification (pWPS) identifies the proposed welding parameters and conditions for the test.
It is prepared by the welding engineer and should follow the relevant requirements of BS EN ISO 15609-1.
The pWPS provides the instructions used to manufacture the qualification test piece.
During welding, the actual parameters are recorded.
The completed test piece is then subjected to the specified non-destructive and destructive examinations.
If the results satisfy the acceptance requirements, a welding procedure qualification record (WPQR) can be issued.
The WPQR documents the successful test and establishes the permitted ranges of qualification.
One WPQR may subsequently support several production welding procedure specifications, provided their parameters remain within the qualified ranges.
Witnessing Requirements
ISO 15614-1 requires the welding and testing activities to be witnessed by an examiner or examining body.
The standard does not automatically require an independent third-party inspection authority.
A suitably qualified employee of the manufacturer may therefore act as the examiner.
However, some clients and application specifications require independent witnessing.
These requirements should be confirmed before testing begins.
Failure to establish the appropriate witnessing arrangements can result in an otherwise satisfactory test being unacceptable for the intended contract.
Essential and Non-Essential Variables
One of the most important aspects of welding procedure qualification is the distinction between essential and non-essential variables.
An essential variable is a welding parameter or condition that can influence the quality or mechanical properties of the joint.
The standard specifies the range within which an essential variable may be changed without requiring another qualification test.
If production welding falls outside that range, further qualification is normally required.
Examples include parent material grouping, material thickness, welding process and certain heat treatment conditions.
Non-essential variables are also recorded in the welding procedure.
They may include joint preparation dimensions, electrode diameter, gas nozzle size, shielding gas flow rate and cleaning methods.
Although these variables do not necessarily require requalification when changed, they remain important to the practical execution of welding.
A production WPS must therefore provide sufficient information for welders to perform the work consistently.
Qualification Test Pieces
ISO 15614-1 specifies test piece configurations and minimum dimensions for different joint types.
These include plate and pipe butt welds, T-butt joints, branch connections and fillet welds.
The test piece must be representative of the welding operation being qualified.
The original article identifies a minimum test piece length of 350 mm.
For expensive materials or thick sections, it may be advantageous to produce a longer test piece than the minimum required.
The unused portion can be retained for possible future testing.
This may be useful if inspection requirements change or additional mechanical testing becomes necessary.
Where the standard test pieces do not adequately represent the intended production weld, qualification based on a pre-production welding test may be appropriate under ISO 15613.
This provides a route for qualifying unusual joint configurations or fabrication arrangements.
Inspection and Mechanical Testing
A successful qualification test must demonstrate that the weld satisfies the specified acceptance criteria.
The testing programme depends on the joint type and applicable requirements.
For a full-penetration butt weld, the examination programme discussed in the original article includes visual inspection, volumetric examination, surface crack detection and mechanical testing.
Non-Destructive Testing
Non-destructive testing is used to identify unacceptable imperfections without destroying the qualification test piece.
Visual testing provides an initial assessment of weld appearance and surface condition.
Radiographic or ultrasonic testing can identify relevant internal imperfections.
Surface examination techniques are used to detect surface-breaking discontinuities.
The required examination methods and acceptance criteria must be selected in accordance with the standard.
The original article refers to quality levels B and C of ISO 5817, as applicable to the relevant imperfection types.
Although ISO 15614-1 does not itself establish a comprehensive personnel certification system for every testing activity, application standards may require NDT personnel to hold appropriate certification under ISO 9712.
The competence of examination personnel should therefore be considered when planning qualification testing.
Transverse Tensile Testing
A transverse tensile specimen includes the weld metal, heat-affected zones and adjacent parent material.
The test evaluates the strength of the welded joint.
The required tensile strength is normally based on the specified minimum ultimate tensile strength of the parent material.
In many cases, failure occurs in the parent material because the deposited weld metal has a higher tensile strength.
However, some high-strength steels present additional considerations.
For example, the original article discusses circumstances involving S960 steel where failure may occur in the weld metal at a lower strength than the parent material.
Such results require consideration of the applicable acceptance provisions and design justification.
Bend Testing
Bend tests provide information about weld ductility and the presence of imperfections.
Depending on the material and joint configuration, face bends, root bends or side bends may be required.
For materials with a specified minimum elongation of 20%, the original article describes bending specimens through 180 degrees around a former with a diameter equal to four times the specimen thickness.
An imperfection exceeding 3 mm in length, as revealed by the bent specimen, is a cause for rejection under the stated requirements.
The correct specimen preparation and test conditions are essential to obtaining meaningful results.
Charpy Impact Testing
Impact testing may be required when the parent material specification, application standard or contract calls for specified toughness.
Charpy V-notch testing is used to assess resistance to brittle fracture under defined test conditions.
The original article describes the removal of three specimens from the weld metal and three from the heat-affected zone.
For joints exceeding 50 mm in thickness, additional specimen sets are required from the root region and adjacent heat-affected zone.
The specified test temperature and minimum absorbed energy depend on the material and applicable requirements.
These tests are particularly important where structures may experience low service temperatures or where fracture toughness is a significant design consideration.
Hardness Testing
Hardness testing can be required to establish whether the weld and heat-affected zone have developed unacceptable hardness levels.
The original article identifies Vickers hardness testing requirements for ferritic steels.
It notes that the corresponding hardness testing is not required for austenitic stainless steels and nickel alloys under the provisions discussed.
Measurements are taken across the parent material, heat-affected zones and weld metal.
The permitted hardness values depend on the material and whether the joint is examined in the as-welded or post-weld heat-treated condition.
Retesting Following Failure
A failed qualification test does not always mean that the entire procedure qualification process must begin again.
ISO 15614-1 contains provisions for retesting in defined circumstances.
Where a test piece fails to meet non-destructive examination requirements, an additional test piece may be welded.
If an individual mechanical test specimen fails, the standard may permit additional specimens to be tested.
The original article notes that two additional mechanical test specimens may be taken under the relevant provisions.
However, retesting is subject to specific conditions.
The precise requirements must be checked before deciding whether the qualification can be accepted.
Parent Material Grouping
Parent material grouping is one of the most useful features of welding procedure qualification.
Rather than requiring a separate test for every steel grade, materials with similar characteristics are assigned to groups.
The grouping system is described in ISO/TR 15608.
The permitted qualification ranges allow one successful test to support welding of several related materials.
For example, the original article explains that qualification using an S355 steel test piece can also provide qualification for S235 and S275 steels within the applicable grouping rules.
It also describes how qualification of certain Group 3 steels can extend to Group 1 and Group 2 materials.
However, filler metal composition remains an essential variable.
The parent material grouping rules must therefore be considered alongside the requirements governing consumables and other welding parameters.
Material Thickness and Qualification Range
Selecting the correct test piece thickness is an important means of obtaining the widest practical qualification range.
The approved thickness range depends on whether the weld is produced using single-pass or multi-pass techniques.
For example, the original article describes a 15 mm thick single-pass joint qualifying a thickness range from 0.5t to 1.1t.
For a multi-pass joint of the same thickness, the corresponding range is 0.5t to 2t.
Here, t represents the thickness of the qualification test piece.
This distinction can have a substantial effect on the usefulness of the resulting WPQR.
Optimising Test Piece Thickness
A 25 mm thick multi-pass qualification test can provide a thickness range from 12.5 mm to 50 mm.
Similarly, a 100 mm thick test piece can qualify a range from 50 mm to 200 mm.
Consequently, two carefully selected qualification tests may cover production welding across a broad range of material thicknesses.
However, increasing the production thickness may require changes to preheat or other welding conditions.
The qualified thickness range must therefore be considered alongside the remaining essential variables.
The standard also places requirements on the thickness of deposited weld metal where more than one welding process is used.
These provisions must be reviewed when qualifying combined welding procedures.
Fillet Weld Qualification
Fillet welds are widely used in structural fabrication.
ISO 15614-1 contains specific rules governing the qualification of these joints.
A butt weld procedure qualification may support fillet welding within the permitted scope.
However, where fillet welding represents the predominant form of welded connection, qualification of fillet welds is required.
The original article highlights opportunities to reduce the number of test pieces by selecting an appropriate T-joint configuration.
A 30 mm thick T-joint incorporating single-pass welding on one side and multi-pass welding on the other may provide broad qualification coverage for fillet welds in material thicknesses above 5 mm.
Such an approach can reduce qualification costs where a manufacturer routinely produces fillet welds of different sizes.
Nevertheless, the precise qualification range must be established using the relevant provisions of the standard.
Pipe Diameter and Branch Connections
Pipe welding introduces additional essential variables.
The original article describes the general qualification range for pipe diameter as extending from 0.5D to flat plate, where D is the diameter of the qualification test pipe.
Selecting a relatively small test diameter can therefore provide a broad range of qualification.
However, the pipe wall thickness must also be considered.
Branch angle is another essential variable.
A qualification test using a 90-degree branch can provide approval for branch angles between 60 and 90 degrees.
Smaller branch angles require separate consideration.
The article suggests that selecting a suitably small branch angle for qualification can maximise the range of production joints covered.
Welding Process and Degree of Mechanisation
A welding procedure qualification is specific to the welding process used.
For example, qualification using manual metal arc welding does not automatically qualify gas metal arc welding or another process.
The original article also distinguishes between manual, partly mechanised, fully mechanised and automated welding.
These operating methods require separate qualification under the provisions discussed.
Manufacturers planning to introduce mechanisation or automation must therefore consider whether their existing procedure qualifications remain applicable.
A change in production equipment may require a new qualification even when the parent material and joint geometry remain unchanged.
Welding Position and Heat Input
Welding position can influence the thermal cycle and mechanical properties of a welded joint.
The original article explains that, where neither hardness nor impact testing is specified, one welding position generally qualifies other positions, with the exception of vertical-down welding.
The PG vertical-down position requires separate qualification.
Where hardness or impact testing is required, heat input becomes an essential variable.
The qualification test must then address the relevant extremes of heat input.
Hardness testing is associated with the lowest heat input condition, while impact testing is associated with the highest.
The original article identifies a 45-degree inclined pipe butt weld, designated H-L045, as one means of producing a test that encompasses different heat input conditions.
Under the provisions discussed, the approved heat input range is ±25%.
This restriction must be considered when preparing production welding procedures.
Preheat and Interpass Temperature
Preheat is an important welding parameter, particularly for ferritic steels susceptible to hydrogen-assisted cracking.
The required temperature depends on factors such as material composition, thickness, hydrogen content and welding heat input.
The original article explains that a reduction in qualified preheat temperature may be possible in defined circumstances.
These include reductions in production material thickness, lower carbon equivalent or changes in heat input.
Any reduction must be justified using the relevant recommendations of ISO/TR 17671-2.
The article identifies a maximum potential reduction of 50°C under the applicable provisions.
Such reductions should not be made solely on the basis of production convenience.
They require a technical assessment of the conditions governing the risk of cracking.
Post-Weld Heat Treatment
Post-weld heat treatment (PWHT) may be required to modify weld properties, reduce residual stresses or satisfy material and application requirements.
The original article emphasises that adding or removing PWHT requires requalification.
PWHT temperature is an essential variable.
The article also notes that the time at temperature is not treated in the same way under the provisions discussed.
Where appropriate, allowing a sufficiently long minimum holding time during qualification may provide flexibility if a component subsequently requires another heat-treatment cycle.
However, the actual heat-treatment conditions must remain compatible with the material and applicable requirements.
Post-heating should not be confused with PWHT.
The two operations serve different purposes and are treated differently within the qualification rules.
Process-Specific Essential Variables
BS EN ISO 15614-1 contains additional requirements for individual welding processes.
The original article highlights several examples.
For continuously wire-fed processes, changing the number of wires or introducing or removing hot or cold wire additions can require requalification.
Flux type is an essential variable for processes such as manual metal arc, submerged arc and flux cored arc welding.
Changes between acid and basic flux systems, or changes in flux basicity, can therefore affect qualification.
Shielding gas composition is also an essential variable for gas-shielded processes.
For metal active gas and metal cored arc welding, the metal transfer mode must be considered.
The article notes that dip transfer qualifies dip transfer only, while spray transfer can provide qualification for spray, pulsed and globular transfer within the applicable rules.
For TIG and plasma arc welding, changing between welding with and without filler wire is an essential variable.
Backing gas arrangements can also influence qualification.
A butt weld qualified without a gas back purge may qualify a procedure using a back purge, but a qualification test performed with back purging does not automatically qualify welding without it.
These examples illustrate why process-specific requirements must be checked when developing a production WPS.
The Welding Procedure Qualification Record
Following successful testing, the examiner prepares the WPQR.
This document provides the formal evidence that the procedure has been qualified.
The original article identifies three principal components.
The first is the qualification certificate, which lists the essential variables and their approved ranges.
The second is a record of the welding consumables and parameters used during the qualification test.
The third is a summary of the non-destructive and mechanical testing performed.
Supporting documents may also include inspection reports, mechanical test certificates, macrographs and parent material and consumable certificates.
The WPQR must provide a traceable record of the qualification.
Validity of the WPQR
The original article explains that there is no fixed time limit on the validity of a WPQR under the provisions discussed.
A successful qualification can therefore continue to support production welding procedures, provided the applicable requirements remain satisfied.
Any number of WPSs may be prepared from the supporting WPQR.
However, each WPS must identify the qualification record on which it is based and include the essential and non-essential variables required for production.
A WPQR is therefore not simply a test certificate.
It is the foundation for controlled welding instructions that can be applied consistently across manufacturing operations.
Practical Considerations for Manufacturers
Welding procedure qualification can involve substantial costs.
These may include materials, welding labour, consumables, non-destructive testing, mechanical testing and witnessing.
For thick or highly alloyed materials, the cost of a single qualification test can be considerable.
Careful planning is therefore essential.
Before testing, the welding engineer should identify the expected production requirements and determine the most useful combination of test piece material, thickness, joint configuration and welding parameters.
The objective is to obtain sufficient qualification coverage without carrying out unnecessary tests.
However, attempts to maximise qualification ranges must not compromise the technical suitability of the procedure.
Preheat, heat input, filler metal selection and other essential variables must remain appropriate for the intended production welds.
The most economical qualification strategy is one that provides both adequate coverage and reliable welding performance.
Conclusion
BS EN ISO 15614-1 provides a structured method of demonstrating that a welding procedure can produce joints satisfying specified quality and mechanical property requirements.
Successful qualification requires more than producing an acceptable weld.
The manufacturer must understand the relevant essential variables, select suitable test pieces, complete the required examinations and document the results accurately.
Careful selection of parent material groups, thicknesses and joint configurations can allow a relatively small number of qualification tests to support a wide range of production activities.
However, the limits of qualification must always be respected.
Changes to welding process, heat treatment, consumables or other essential variables may require further testing.
The WPQR provides the evidence supporting production welding procedures, while the WPS translates that evidence into practical instructions for welders.
As with any technical standard, the precise requirements must be checked against the applicable edition, contract specification and regulatory obligations.
Failure to do so can result in costly requalification and production delays.
References
-
BS EN ISO 15614-1:2017+A1:2019. Specification and qualification of welding procedures for metallic materials – Welding procedure test – Part 1: Arc and gas welding of steels and arc welding of nickel and nickel alloys.
-
BS EN ISO 15609-1:2019. Specification and qualification of welding procedures for metallic materials – Welding procedure specification – Arc welding.
-
BS EN ISO 15613:2004. Specification and qualification of welding procedures for metallic materials – Qualification based on pre-production welding test.
-
BS EN ISO 5817:2014. Welding – Fusion-welded joints in steel, nickel, titanium and their alloys – Quality levels for imperfections.
-
BS EN ISO 9712:2012. Non-destructive testing – Qualification and certification of NDT personnel.
-
PD CEN ISO/TR 15608:2017. Welding – Guidelines for a metallic materials grouping system.
-
ISO/TR 17671-2:2002. Welding – Recommendations for welding of metallic materials – Arc welding of ferritic steels.
-
ASME BPVC Section IX, 2023. Welding, Brazing, and Fusing Qualifications.
Original publication: Welding and Joining Matters, Issue 11, April 2025, pages 18–22.
Original author: EUR ING Gen Mathers CEng MSc DiplIM FWeldI.
Editorial note: This article is a newly written website adaptation of the original Back to Basics feature. The technical requirements reflect the standards and editions discussed in the April 2025 publication. It is not a substitute for the applicable standard, and technical and editorial approval should be obtained before publication under the original author's byline.